Anodizing Aluminum

Steps:
Put on gloves and goggles
Clean and degrease part
Desmut in lye water (Draino, Liquid Plumr) 2-3 mins
Rinse in distilled water
Wipe off the smut (black stuff) with wet paper towel or toothbrush
Prepare acid 19% and let cool
Anodize 1-2 hours
Rinse in distilled water
Die 2-20mins 90°F
Seal in boiling water 30-60 mins

If you don't like the finish you can remove the anodized layer by putting it back in the lye water (Draino, Liquid Plumr) for 5-10 mins.

Thanks for watching,
Russ
Anodizing AluminumPMBO 2013 #5- (Update) EMF Charges Capacitor to 7 Volts!!!Our Version of the Chicken TractorLaser EPG 014 - Finished Magnetizing Chamber & New Direction of the Magnetic Gas ProcessorEPG Tests 003 - Hydrogen (H2) & Oxygen (O2) Through a Magnetic FieldLaser EPG 020 - Magnetic Gas Production PossibilitiesExplanation Attracting Elytra  - Grebennikov Video Replication SeriesPMBO 2013 - WinnersViktor Grebennikov #1 - Testing Scarab (June Bug) Wing CoversLaser EPG 007 - HGG Hydrogen Gas Gun/Processor Part 4, Testing Spiral Design (CORONA DISCHARGE)